Skip to content
Inytialgo

Process 10 min read

Aluminium die casting defects: how to read them and what to fix

By Inytialgo ·

Filling simulation of a ring-shaped part: the red metal front enters through the runner and gates while the rest of the cavity is still empty

Aluminium die casting defects fall into three families: internal (gas porosity, shrinkage porosity, inclusions), surface (cold shuts, soldering, blisters, flash) and dimensional (distortion and parts out of tolerance). Each one is traced to its cause the same way: classify the defect by its morphology and its occurrence, correlate it with the process parameters and attack the cause, not the symptom. The name on a scrap tag says what the part looks like, not why it happened, so in aluminum high pressure die casting (HPDC) the reading comes before the correction.

How to read a die casting defect before you name it

Morphology is the shape and location of the defect. A rounded pore and a branched cavity in a thick boss are both called porosity, but the first is usually gas and the second shrinkage.

Occurrence is the pattern over shots and cavities:

  • Same place, every shot. The cause is usually built into the part or the die: geometry, gating, a hot spot. The die and the gating system write the result, as we explain in how the die casting process works; changing the shot profile only moves the defect around.
  • Random places, some shots. Process variation: metal temperature, die temperature after a stop, spray volume, a drifting shot profile.
  • One cavity of a multi-cavity die. Look at what is different about that cavity: runner length, overflows, cooling circuit.

Then put the defect next to the shot log. If it peaks after a stop and fades as the die heats, it is thermal; if it follows a parameter, that parameter tells you where to look.

We recommend recording occurrence before touching the machine, because a correction made on a random defect as if it were systematic changes two things at once, and nobody can tell afterwards which one worked.

Aluminium die casting defects at a glance

The European classification, CEN/TR 16749:2014, sorts defects first by location: internal, external (surface) and geometrical, meaning dimensions and tolerances. The families below are the standard’s; placing each of these high pressure die casting defects in one of them is our reading. Each row gives the usual causes and solutions as a starting point, and occurrence decides between causes.

Defect Family How it looks Usual cause What gets corrected
Gas porosity Internal Rounded pores at the end of the fill Air, steam or gas trapped during filling Venting, overflows, first phase, spray volume, vacuum
Shrinkage porosity Internal Irregular, branched cavities in thick sections Contraction with no liquid metal left to feed it Local cooling, wall thickness, intensification timing
Inclusions Internal Hard spots or oxide films when machining Oxides and residue carried in with the metal Melt cleaning, ladling, plunger lubricant
Cold shut Surface Seam where two metal fronts met without fusing Cold metal, slow shot or cold die Fill time, gate position, die temperature, overflows
Soldering Surface Torn, rough patch; aluminum stuck to the die Alloy reacting with the iron of the die steel Die temperature, spray coverage, alloy iron content
Blisters Surface Bumps that lift the skin, often after heat treatment Gas pores just under the surface Same as gas porosity
Flash Surface Thin fin at the parting line or slides Die opening under pressure, or a worn die Locking force, die position, die maintenance
Hot tear Surface Jagged crack at a corner or change of section Contraction restrained by the die Radii, local cooling, ejection timing
Distortion Geometrical Part out of flatness or out of tolerance Ejection force, uneven die temperature Ejection system, draft, cycle time

Gas or shrinkage: how to tell die casting porosity apart

Aluminum die casting porosity comes in two kinds that look alike on an X-ray and are cured in opposite ways. In a 2020 study of HPDC aluminum, Nourian-Avval and Fatemi (Materials 13(14):3068) describe gas pores as more or less spherical and shrinkage pores as irregular, branched interdendritic cavities, with defect size growing with section thickness. Gas is air, steam and shot sleeve gas trapped during filling, so it gathers where the last air had nowhere to go; shrinkage is contraction with no liquid left to feed it, so it sits in the thick sections that freeze last.

To confirm which one you have, section the part through the defect, look at the cavity shape and check where it sits against the wall thickness. Then change one thing: if the defect moves with the first phase or the venting, it is gas; if it moves with local cooling or die temperature, it is shrinkage.

Gas is fought with venting, overflows, a calmer first phase, less spray and, where the part demands it, vacuum. Shrinkage is fought thermally: local cooling, a more uniform wall, and intensification while the gate can still feed. NADCA’s manual Operating the Die Casting Machine (E-902, 2008) describes blisters as gas porosity trapped near the surface whose pressure lifts the skin.

Two figures from ASTM E505-22: 3 discontinuity categories for each alloy family, aluminum and magnesium, each illustrated in 4 levels of increasing severity
Reference radiographs for inspection of aluminum and magnesium die castings · Source: ASTM International, E505-22 «Standard Reference Radiographs for Inspection of Aluminum and Magnesium Die Castings» (active standard) · Chart: Inytialgo

How much porosity a part may have is an acceptance question, not a process one. ASTM E505-22 provides reference radiographs for aluminum and magnesium die castings: 3 discontinuity categories for each alloy family, each illustrated in 4 levels of increasing severity, with ASTM E2973 for digital X-ray. How those criteria get written on an automotive drawing is covered in automotive die casting.

Cold shuts and misruns in thin walls

A cold shut is a surface imperfection where metal streams fail to fuse, and NADCA’s E-902 manual gives the cause in one line: cold metal, a slow shot or low die temperatures. A misrun is a section that never filled. Both tend to appear far from the gates, on thin walls or where the flow rejoins around a core. In practice, check in this order: fill time (a slow fast-shot or a late switch point), a cold die face after a stop or from local over-spraying (see die lubricant and release agents), and fronts meeting in a corner with no overflow to take the cold first metal.

Thin wall die casting makes every one of these worse. Die casters become reluctant below about 2.5 mm in aluminum alloys, and the limit is not so much filling the cavity once as holding those conditions shot after shot; near that limit, walls and gates are settled at the enclosure design stage.

Soldering and erosion at the gate

Soldering and erosion both damage the die in front of the gate, by different mechanisms. The soldering defect in die casting is the aluminum alloy reacting with the iron in the die steel and forming Fe-Al intermetallic layers: the part comes out with a torn patch and the die keeps aluminum stuck to it. Close to 1% Fe in the alloy is generally believed necessary to reduce it (Winkelman et al., J. Mater. Sci. 39, 2004); the common alloys are compared in aluminum die casting. Erosion attacks the gate area and any surface the metal hits fastest.

Before blaming the alloy, calculate gate velocity. A worked example to redo with your own numbers (a typical case, not a client’s):

  • Plunger diameter 80 mm, fast-shot velocity 2.0 m/s.
  • Plunger area: π × 40² = 5,026.5 mm².
  • Flow: 5,026.5 mm² × 2,000 mm/s = 10,053,096 mm³/s, about 10.05 dm³/s.
  • Gate of 2.0 × 150 mm = 300 mm²: gate velocity = 10,053,096 ÷ 300 = 33,510 mm/s, that is 33.5 m/s.
  • Same gate thinned to 1.5 mm to chase a cold shut, 225 mm²: 44.7 m/s.
Calculation: an 80 mm plunger at 2.0 m/s pushes about 10.05 dm³/s of metal; through a 300 mm² gate that is 33.5 m/s, and through the same gate thinned to 225 mm² it is 44.7 m/s
Gate velocity for an 80 mm plunger at a fast-shot velocity of 2.0 m/s, gate 150 mm wide; typical case, not a client's · Source: Inytialgo calculation: flow = plunger area × plunger velocity; gate velocity = flow ÷ gate area · Chart: Inytialgo

Thinning the gate by half a millimeter raised the metal velocity at the gate by a third. As our guide to die cast tooling puts it, gate velocity that is too high buys you filling at the cost of steel, so check the new gate against the limit your die maker or process sheet works to before machining it.

Flash: a clamping problem or a die problem?

Flash is a thin fin of metal where the die halves meet, along slides and vents or around pins, and where it appears tells you most of the cause:

  • Consistently on the same side of the parting line: clamping. The die opens under metal pressure because the locking force does not cover the projected area at the pressure you use, or because the load sits off-center on the tie bars. The check is in die casting machine types and tonnage.
  • On a slide, a vent or around a pin, getting worse over time: wear or damage in the die. That is a maintenance correction, not a machine one.

A die that leaks metal also gives air a way in and limits the vacuum a vacuum system can reach, which is why our vacuum-assisted die casting approach starts by making the die tight. On the vacuum valves running in plants in Mexico, our founder put it this way: the advantage is double, because rejection goes down and the process can run with less aggressive parameters; you get the same or slightly better rejection, but with much more stability and without flash.

Distortion and dimensional defects

A warped part is a geometrical defect, and in thin-walled aluminum it is often born at ejection rather than in the shot. The hardest moment of the part’s life may be its birth, the extraction from the die: the pins push a part that is still hot, and if the force needed is high, it bends instead of releasing. If the distortion repeats in shape and direction, look at ejection before correcting the die dimensions: pin layout, draft and a plate that flexes. Stiffening the ejector plate and its guiding cut the force to eject a thin part from 8 to 3 tonnes in our ejector plate stiffness case.

Which defects can simulation show before the die is built?

Filling and solidification simulation shows the causes of several aluminum die casting defects before the steel is machined: where air is trapped and fronts meet cold (gas porosity, cold shuts) and which zones freeze last (shrinkage). It does not fix the metal: melt quality, dross and hydrogen are not in the model unless you put them there. In a defect project, casting simulation software confirms the cause the morphology pointed to and tests the correction on screen. We distribute Simcenter Inspire Cast (formerly Altair Inspire Cast) from Siemens Digital Industries Software; the details are on the Simcenter Inspire Cast page.

Where to start with a defect that is already costing scrap

Start with data, before changes: the real parameters on the die casting machine, the defects on the parts, the condition and design of the die, cycle times and cell stoppages. No assumptions, and nothing changed yet. That is the diagnosis stage of our die casting consulting.

For a first proposal, we ask for the drawing or the 3D model of the part, the alloy, the machine tonnage and a description of the defect with photos.

If you want your own plant team to do this reading, our training includes a 16-hour program, Identifying and correcting HPDC defects, delivered in-company or online; the details are on the die casting training page.

  • #aluminium die casting defects
  • #die casting porosity
  • #cold shuts
  • #soldering
  • #HPDC

Found this useful? Add Inytialgo as a preferred source and you'll see our posts more often in your Google Search.

Add as a preferred source on Google